So I got the 0.2mm Nozzle for my P1S to do some Detail Heavy stuff, while with PLA everything works perfectly Fine, Once I try to use any Roll of PETG HF it just refuses to Stick to the Plate!
I’ve been Mostly Testing on my Coolplate Supertack, but same issue happens on the Textured PEI. Both of them have no issues when trying PLA the Print before.
I’ve now tried a Range from 230c° to 250c° for the Nozzle and 60c° to 85c° for the Headbed with only limited result, as Only the Combination of 250c° and 85c° for the Heatbed got me the Brim around the Print to stick, but not the print itself.
What am I overlooking here? Is there some settings I need to adjust when switching Nozzles? Dp I need to go even Higher with the Temps? Maybe its the Flow Ratio? I’ve tried both the reset one and the one that was set with the 0.4 Nozzle with no real change. Cant run a new calibration for it since nothing sticks. Both spools of Filament have been dried for 48 Hours, with a few hours of resting before use ofcourse.
To note, PETG HF works perfectly fine on the 0.4 Nozzle and both Plates have been cleaned multiple times now… as seen to work with PLA. What settings work for you folks? Anyone with simular issues?
All my petg experience is with a .6 nozzle, printing on a glass bed, but there’s some takeaways that hopefully apply to a .2 one…
Going very slow and increasing extrusion width helps a lot. And keeping acceleration low-ish, decreasing travel speed too much doesn’t help ofc. The narrow extrusion of a .2 nozzle reduces the surface area of a single line even more, so probably you need to increase the line width even more.
Additionally, I’ve read somewhere that petg kinda likes to stick to brass but not glass. So having the bed as hot as you can get away with for the first layer and the nozzle as cool helps too.